Mar 01, 2022

1 Jarayon oqimi

The printed circuit board with the prepared graphics → acid degreasing → scanning water washing → secondary countercurrent water washing → micro-etching → scanning water washing → secondary countercurrent water washing → copper plating predip → copper plating → scanning water washing → tin plating predip → Tin plating → secondary countercurrent washing → lower plate

2 batafsil jarayon

2.1 Qalay qoplamasi

2.1.1 Qoplashdan oldingi-qoplamaning tarkibi va ishlash shartlari

2.1.2 Qalay prepreg idishini ochish usuli 4

Avval yarim tsilindr distillangan suv qo'shing, so'ngra asta-sekin suvga botiring va massa ulushi 98 foiz bo'lgan 15 l sulfat kislota qo'shing, aralashtiramiz va sovutib, 1,5 litr Sulfotech A qismi qo'shing, bir tekis aralashtiramiz, 300 litrgacha distillangan suv qo'shing, teng ravishda aralashtiramiz va u foydalanishga tayyor.

2.1.3 Cho'milishdan oldingi-qalay{3}}qoplamaga texnik xizmat ko'rsatish va nazorat qilish

Har bir 100 m2 taxta uchun 1 litr sulfat kislota va 100 ml Sulfotech A qismi qo'shing. Hammom har safar 1500 m2 plitalarni qayta ishlaganda hammomni almashtiring.

2.2 Qalay qoplama

2.2.1 Qalay qoplamali eritmaning tarkibi va ishlash shartlari 5

2.2.2 Kalayli idishni ochish usuli 2

Avval yarim tsilindr distillangan suv qo'shing, so'ngra asta-sekin massa ulushi 98% bo'lgan 98 l sulfat kislota qo'shing, aralashtiramiz va sovutgandan so'ng, 25 gradusgacha sovutish uchun 40 kg qalay tuzi 235 qo'shing, 76 l Sulfotech qismi A, 15,2 l Solfotech qismi qo'shing. B, 30,4 LSTHadditive Sulfolyt, Suyuqlik darajasiga distillangan suv qo'shing va aylantiring (1,5A/dm2 da 2AH/L elektroliz qiling).

2.2.3 Qalay qoplamali vanna suyuqligiga xizmat ko'rsatish va nazorat qilish

Ishdan oldin qalay va sulfat kislotani tahlil qiling. Har bir 100 m2 plastinka uchun 11 l sulfat kislota, 600 g qalay tuzi 235, 600 ml Sulfotech A qismi, 800 ml Sulfotech B qismi, 750 ml STH qo'shimchasi sulfolit qo'shilishi kerak. Avtomatik qo'shish tizimi 200AH da 56 ml Sulfotech A Part qo'shdi.

Sulfotech Part A va Sulfotech Part B ni kuzatish va sozlash uchun eritma har hafta Hull hujayra sinovidan o'tkazilishi kerak.

Buyum doirasi Eng yaxshi qiymat

Sn2 plus 20-30 ml/L 24 ml/L

Vt(H2SO4) 98 foiz 160-185mL/L 175mL/L

Sulfotech A qismi (Sulfotech A qismi) 30-60mL/L 40mL/L

STH (STH qo'shimchasi sulfolit) 30-80mL/L 40mL/L

Sulfotech qismi B 15-25mL/L 20mL/L

Ishlash harorati 18-25 daraja 22 daraja

Katod oqimining zichligi 1,3-2.ASD 1,7ASD 2